Densimetric table: test on copper cable granulate

Item Details
Laboratory StokkermillLab – Seltek S.r.l., Udine (Italy)
Test dates 16 November 2026; refinement of sample C2: 19 November 2026
Material Copper electrical cable granulate, 2 samples (C1, C2)
Equipment Stokkermill laboratory density table; conveyor belt with magnet; 2 mm screen
Type of assessment Qualitative, by visual inspection on an A4 reference background

Summary: density separation of copper cable granulate

The Stokkermill laboratory density table separated both cable granulate samples into a heavy fraction of clean copper and a light fraction with no visible copper. The result also holds for sample C2, which is rich in textile fibres and insulation. On the C2 copper, an additional pass over a magnet and a 2 mm screen removed the ferrous parts and the larger mixed pieces, further increasing the visual purity of the product.

1. Introduction: cable recycling and density separation of copper

Electrical cable recycling is one of the main sources of non-ferrous metal recovery. After shredding and granulation, the material is a heterogeneous mixture of copper, plastic insulation (PVC, polyethylene), rubber, textile fibres and dust. The economic value of the product depends on how well the copper is separated from these components.

Density separation exploits differences in the specific gravity and aerodynamic behaviour of particles. On an inclined, vibrating deck crossed by an adjustable air flow, light particles are fluidised and migrate towards the rear outlet. Heavy particles stay in contact with the deck and are conveyed towards the front outlet. The process is entirely dry.

The aim of the test is to verify the separability of two cable granulates of different composition on the Stokkermill laboratory density table. A secondary aim is to assess the improvement in purity achievable with downstream magnetic separation and screening.

2. Materials and methods of the laboratory test

2.1 Copper cable granulate samples

Code Description of the input material
C1 Typical granulate from cable shredding and granulation: thin, curly copper wire, coloured PVC and rubber sheaths, fibres and fine dust. High copper content.
C2 Lighter, more heterogeneous granulate: large flakes of insulation, textile and fibrous material, coloured sheaths and dust. Visibly lower copper content than C1.

2.2 Equipment: laboratory density table, magnet and screen

  • Stokkermill laboratory density table, with front outlet (heavy fraction) and rear outlet (light fraction).
  • Conveyor belt with magnet, to remove ferrous parts.
  • Screen with 2 mm aperture, for particle-size classification of the copper.

2.3 Test procedure

  1. Each sample was fed onto the density table. Air flow, vibration and deck inclination were adjusted by the operator for the individual material.
  2. The fractions at the front and rear outlets were collected separately.
  3. The heavy fraction of C2 was passed over the conveyor belt with magnet.
  4. The non-magnetic fraction was screened at 2 mm, producing an undersize and an oversize.
  5. Inputs and fractions were photographed on the same Stokkermill A4 sheet, used as a reference background for visual comparison.

2.4 Test flow chart

Flow chart of the density separation test on copper cable granulate with coded fractions
Test flow chart · coded fractions

C1 was processed on the table only; C2 continued with magnet and screen. The fraction codes are used in the figures and in the results table.

3. Density separation results

3.1 Sample C1 – high-copper granulate

On the first pass over the table, C1 separated into two distinct fractions. The heavy fraction consists almost entirely of copper; the light fraction shows no visible copper wires.

Mixed copper cable granulate before separation on the density table
Figure 1 – C1, input material. Thin, curly copper wire still mixed with insulation, coloured PVC and rubber sheaths, fibres and fine dust.
Clean copper at the front outlet of the Stokkermill density table, sample 1
Figure 2 – C1-P, heavy fraction (front outlet). Bright copper wire, with no visible insulation, fibres or dust. Only a few small metal flakes present.
Light fraction of plastic and dust with no copper, rear outlet of the density table
Figure 3 – C1-L, light fraction (rear outlet). Dark plastic granules, fibres and fine dust with small fragments of coloured insulation. No visible copper wire: metal loss in the reject negligible on visual inspection.

3.2 Sample C2 – heterogeneous granulate rich in fibres and insulation

C2 represents a more demanding working condition: textile fibres and insulation flakes tend to trap the fine copper wire. Despite this, the table produced a heavy fraction of clean copper and a light fraction with no significant copper.

Cable granulate rich in fibres and sheaths, sample 2 input
Figure 4 – C2, input material. Large flakes of insulation and textile or fibrous material, coloured sheaths and dust. Visibly lower copper content than C1.
Copper separated by the density table from fibrous granulate, sample 2
Figure 5 – C2-P, heavy fraction (front outlet). Fine, curly copper wire, free of insulation and dust. A few heavier metal fragments (tinned or brass) correctly concentrate in this fraction.
Light reject of insulation and textile fibres with no copper, sample 2
Figure 6 – C2-L, light fraction (rear outlet). Insulation flakes, textile fibres, coloured plastic particles and dust. No significant amount of copper wire visible.

3.3 Refining C2-P: magnetic separation and 2 mm screening

The heavy fraction C2-P was treated in two successive stages: removal of ferrous parts on a belt with magnet, then classification on a 2 mm screen. The undersize is the product with the highest visual purity of the entire test.

Ferrous parts removed from the copper with belt and magnetic separator
Figure 7 – C2-Fe, magnetic fraction. A few small pieces of steel, such as clips and terminal fragments, held by the magnet.
High-purity fine copper after 2 mm screening
Figure 8 – C2-P < 2 mm, undersize. Fine, curly copper wire, practically free of insulation, fibres, dust and ferrous parts. Visually higher purity than C2-P (figure 5).
Oversize above 2 mm with copper tangles and brass contacts
Figure 9 – C2-P > 2 mm, oversize. Tangles of copper wire with heavier non-ferrous pieces (brass and tinned contacts) and some insulation residue. Small share of the total, recoverable separately or for reprocessing.

3.4 Summary of the separated fractions

Code Stage Observed composition Destination
C1-P Table, front outlet Almost pure copper, a few metal flakes Product: copper
C1-L Table, rear outlet Plastic, fibres, dust; copper not visible Light reject
C2-P Table, front outlet Clean fine copper, some brass/tinned fragments To refining
C2-L Table, rear outlet Insulation, textile fibres, plastic, dust; copper not significant Light reject
C2-Fe Magnet Steel clips and terminal fragments Ferrous
C2-P < 2 mm Screen, undersize Fine copper, practically free of impurities Product: high-purity copper
C2-P > 2 mm Screen, oversize Copper tangles, brass, tinned parts, insulation residue Separate sale or reprocessing

4. Discussion: why copper separates from plastic and fibres

The behaviour of the two samples confirms the principle of density separation. Copper, with a specific gravity of about 8.9 g/cm³, is much denser than PVC, rubber and textile fibres, which typically stay below 1.5 g/cm³. This wide gap allows a clean separation even with small quantities and irregular particle sizes.

The expected critical issue for C2 was fine copper wire being carried over by the fibres, which form light agglomerates. Fraction C2-L shows no significant copper: adjusting the air and vibration proved sufficient to free the metal from the fibres.

The downstream stages act on impurities that the table, by principle, cannot separate. Heavy metals other than copper (steel, brass, tinned contacts) have similar or higher density and end up in the heavy fraction. The magnet removes the ferrous share; the 2 mm screen isolates the larger non-ferrous pieces and agglomerates, leaving the purest fine wire in the undersize.

5. Conclusions of the density table test

  1. The Stokkermill laboratory density table separated both granulates into a clean copper fraction and a light fraction with no significant copper.
  2. The result is confirmed on sample C2 too, which is heterogeneous and rich in fibres and insulation.
  3. Magnetic separation and 2 mm screening downstream of the table remove the remaining ferrous parts and the larger mixed pieces, bringing the fine copper to the highest visual purity.
  4. The materials tested are suitable for processing on a Stokkermill cable recycling line with density table. Magnet and screen are a recommended option when maximum copper quality is the goal.

6. Test limitations and next steps

The assessment is qualitative: the fractions were compared by visual inspection, without weighing or chemical analysis. No mass balance, copper recovery yield or metal content in the reject is therefore reported. The test is at laboratory scale and on limited sample quantities.

For a full characterisation, StokkermillLab can carry out on request:

  • weighing of input and fractions, with mass balance and recovery yield;
  • determination of the copper content in the light fraction, to quantify losses;
  • recording of the table’s adjustment parameters, as a basis for sizing the industrial line.

Request a StokkermillLab separation test

Every cable granulate has its own composition. The Stokkermill laboratory in Udine processes real samples, assesses the separability of the material and identifies the plant configuration best suited to production. Write to info@stokkermill.com or visit www.stokkermill.com to arrange a test.

23/11/2026